Spectrometer sampling from melts

    Directions and specification are available for all possible methods of sampling from all possible materials. For sampling metals and in particular molten metals such as pig iron, cast iron and steel, reference is made to /226/, and for non-ferrous metal /227/. Selected sampling procedures for precious metals are described in /228/.

    These samples are used to monitor the molten metal and must be taken, prepared and examined quickly; we speak of preliminary and final samples.

    The sampling method for spectrometers with SDAR can be simplified and standardized by meeting the following requirements:

   a)  The sample must be representative of the melt.

   b)  The elements must be evenly distributed so that the effective sample of about 1 mg will give a reliable value for the composition. The sample must be suitable for use as an electrode in the discharge gap ie. It should have few and small precipitates. Geometric dimensions must be suited to the sample stands designed for cast samples.

   c)  Samples should not have slag inclusions or cracks.

   d)  Chill mould handing should be simple.

   e)  Sample preparation should be simple.

   Re a) The correct time for sampling is sampling is important. After master alloys have been added. It is necessary to wait until a homogeneous melt has formed. When oxidized scrap is added it is necessary to wait until the oxygen has left the metal bath in the form of oxides.

   Re b ) This requirement is often met by casting minimum-weight analysis samples at cooling rates up to 50°C/s. As the sample mass grows with the square of diameter, it should be as small as possible. A diameter of 25-30 mm is sufficient for 4 burn spots. The sample is usually taken in two steps: the liquid sample is removed from the melt and transferred to the mould.

   During sample-taking, the spoon is coated with the slag floating on the bath in order to prevent reaction between the spoon and the liquid metal and to heat the spoon in order to avoid premature solidification of the sample. The spoon can also be coated with mould wash, dried and preheated; the slag coating can then be dispensed with. The sample material should be hot when poured into the mould in order to ensure a reliable flow. The mould should be near the sampling point, and pouring should take place quickly in order to avoid heat loss. The spoon must not be set down during pouring as this will give rise to cold shuts which require additional sample preparation work. It is also assumed threat cold shuts cause breaking-up at the burn spots since heat conduction to the dense part of the sample is made more difficult. To ensure a reliable flow into the mould the riser should be poured full to increase the inlet pressure.

   The interior of the mould must be metallically bright using a brass brush. Cu moulds with oxidized inert surfaces become ineffective for rapid heat conduction. In pig iron and cast iron samples this may lead to precipitation of free C. The interior must be cleaned after about 20 samples.

   It is recommended that there should be no water cooling, because of condensation. At each sampling point there should be number of moulds which can be used in succession.

   With moulds made of soft or haematite iron or cast iron. Because of poor heat dissipation local melting of the mould material occurs where sample and mould become welded together. When the sample is removed the mould splits at these points. These moulds are suitable for non-ferrous metals with lower melting points. Low melting point metals may have segregations from high melting point metals due to slow cooling, so special care must be taken to have a high cooling rate to obtain homogeneous samples.

   Re c) This requirements can only be met by the sampler’s skill. The slag floating on the sample material in the spoon can be largely removed by pouring back some of the spoon contents with a jerky movement into the melt or by skimming it with a slag knife.

   The sampler should wear blue goggles during sampling so as not to make excessive demands on his eyes. Because of its higher optical emission coefficient he can distinguish the slag from the metal and prevent it from flowing into the mould. Fig. shows Al samples with and without inclusions. Sample a cannot be used for spectrochemical analyses.

   Unkilled steels must be deoxidized. After the slag skin has been removed, Al or Zr is added to be spoon in unit lengths. Deoxidation in the mould is not advisable since the agent may be dissolved before the melt solidifies.

   Rapid cooling is desirable for reasons connected with homogeneity and to obtain small precipitates.

   Oxygen-containing copper with >0.05% oxygen leads to porous samples during casting and to incorrect analyses with SDAR. Effective killing can be achieved by adding CuP10-1/200th of sample weight. Care must be taken to ensure that contamination introduced to the sample by impurities from the deoxidizing agent does not cause interference. If they do cause interference this must be taken into account during calibration.

   When not in use, moulds should lie on one side or be covered to that no dirt can enter them.

   Some qualities of materials become cracked become cracked or break up if they are quenched in water from deep red heat. Cast iron samples with phosphorus concentration >0.15% must be removed from the mould after <10s and cooled in air or by compressed air. If they are left 15s in the mould like other cast iron samples they often break up because of high internal stresses. Sample transport to the laboratory can be included in the cooling time if steel containers are used.

  Mould shape and sample dimensions once differed widely. The shapes most widely used for ferrous and non-ferrous metals were cylindrical with a diameter of about 35mm and a height of 50-100mm. Sample weights were 0.5-1kg and the mean cooling rate was a few ℃/ s.

   Steel samples with relatively large quantities of precipitates eg. MnS  were cut to expose the bottom third using expensive cutting machines. In this region the distribution of the precipitates is, to some degree. homogeneous. The size distribution of the MnS precipitates from the base upwards is as shown in Fig. 5.5. The chemical concentration of manganese and sulphur below the solidification shrinkage cavity is the same all over. Since intensities were formerly measured before the SS was reached, they increased with increasing MnS ?. For many years the “best part”of the sample was cut off, namely the bottom part with small precipitates.

    For pig iron and cast iron a wider range of mould shapes was used than for steel.  All efforts were concentrated on obtaining small analysis samples with high cooling rates, as was and still is obligatory because of the risk of free carbon precipitation.

    Samples from non-ferrous metal were often cast in a “mushroom-shape” but the diameter of the analysis was often large than necessary.

On the basis of these requirements and explanations, sampling can be simplified as follows:

    1. Metal with small precipitates and little tendency towards segregation can be cast in Mould. A ring 25 mm high with an internal diameter of 30mm lies on a copper plate at least 1 cm thick with a metallically bright surface. The ring is made of high-alloy steel or ceramic so that heat is mainly conducted into the copper plate. This gives rise to directed structure with good homogeneity over the surface of the sample. Vertical homogeneity must be tested.

Mould is suitable for the following metals:

Pure metals

Genuine hypoeutectic metal alloy eg. CuZn, CuNi, ZnAl.

   Test on steel with 0.06% S have shown that samples from Mould 1 are homogeneous over at least 10mm from the base. These steel samples, after grinding, are ready for analysis. A cutting machine is not required. Much the same applies to the most alloys on Ni and Co bases. Fig 5.8 also shows 4 samples taken from this mould. The samples can be removed from the ring after 25s.

   2. Metal with large precipitates and a tendency towards segregations should be cast . The samples thus obtained are 6mm thick and about 30mm ?.  The upper part can be cast iron. The riser and underside of the upper part should have oxidized surfaces so that the liquid samples flows into the analysis sample shape as far as possible without cooling. The analytical sample mould must be brushed bright by regular use of a brass brush in order to ensure rapid directional solidification. The cooling rate is about 25°C/s. The samples can be removed from the mould after about 15 s is necessary to reach the SS. If the same material is cast into Mould fine droplets are obtained and a pre-spark time of 30 s is sufficient. The samples with large precipitates give poor calibration and excessively high intensity. Samples with precipitation sizes different from the foregoing lead to incorrect analysis results. 

   All types of sample in group 1 can be cast in the Mould , but manipulation of Mould 1 is easier.

   Samples which require a high cooling rate in order to suppress precipitates can be cast. Their thickness is 3-4mm, ? about 30 mm and their weight is 1.5 times less than the weight of samples from Mould. The analysis sample has a cooling rate of about 50°C/s and can be removed from the mould after about 15s.

    Pig iron and mixer metal, cast iron, malleable iron and nodular cast iron.

    Most samples have solidification hollows on their underside which, if the riser is at the centre, should be removed by grinding. If the hollow is at the edge it need not be ground-out as there is still sufficient surface for 4 burn spots. There is less risk of cold shuts occurring with this mould than with top pouring. Cooling is sufficient. With a C equivalent of:

C eq=%C +1/3(%Si+%P)<5.0,

equivalent to a degree of saturation S =5.0/4.2=1.2, to prevent grey solidification. In nuclei-rich iron grey solidification is promoted, but is retarded if carbide-forming agents are present. Grey solidification can be recognized in the fracture or form the C burn-off curves. Metallically bright mould interiors and additions of elements suppressing grey solidification promote white solidification.

    A mould developed by Georg Fischer Foundry, Schaffhausen CH, for sampling cast iron consist of a solid Cu block with openings on both sides Cu block with openings on both sides for the analysis sample which is 25 mm ? and 5 mm thick.          The sample material is poured through an insulating sand core in order to reach the opening while still as hot as possible.        

   The riser can be knocked off. The underside of the opening must be kept metallically bright by regular use of brass brush.      

    The mould can easily be remachined.

    The cooling rate can be increased by casting pin samples. The samples is 40mm long, 6 mm in ?, and the weight of the analysis sample is 8 g. Compared with this, the weight of the coin-type disc sample from Mould 3 is 30 g.

    A large number of cast iron samples cast in parallel as 4 mm coins and 6 mm pins with Ceq <5.0 show free C in the fracture for 65% of the coins. The pins were all graghite-free. The pin sample has the advantage that sample fracture is part of the sample preparation process and free C is detected. If the sample contains graphite, then either an analysis programme with a longer pre-spark time should be adopted; the sample should be discarded; or it should be homogenized in a further sample preparation stage. Sample preparation for the pin sample is simpler and faster than for the coin sample. As pin samples always have the same ?, they can easily be fitted into a special holder. Except for sulphur, the same calibration curves are obtained as for coin samples, so that calibration can be carried out with coin reference samples. In precision and accuracy they are comparable with coin samples. Due to the poor thermal conductivity of these cast iron samples pre-sparking should be carried out with discharge parameters which do not lead to thermal overloading of the sample surface.

   In hypereutectic alloys precipitation is often already present in the melt and increasingly so as the temperature approaches the solidification temperature. This applies eg. to precipitated carbon in hypereutectic cast iron. This precipitated carbon is not detected during thermal analysis as it does not affect the holding temperature. When the sample is crushed for chemical analysis, its precipitates turn to powder, leading to low analysis values. ues. Pig iron which contains graphite foam in the run-off channel does not acquire a white structure even with rapid cooling. Coin and pin samples from such material contain graphite foam over their cross-section. Such samples should be prepared by remelting in separate furnaces, possibly with a pure iron addition in order to reduce the C eq.

   There are alloys, however, which show considerable segregation even at cooling rates >50°C/s. Examples are Al alloys with a few percent of Cu. In these cases pouring at a high cooling rate would lead to analysis samples which are far from homogeneous. For this reason they are poured into Mould in order to find a region which is homogeneous over some mm from the base of the sample outwards. This region is the analysis zone of the analysis sample which has to be stated and adhered to in subsequent analyses. The concentration in this zone need not correspond to the mean bulk concentration (that of the but it is proportional to it. For this reason, calibration curves plotted from calibration samples must be given a corresponding factor.

   Because of the concentration gradient a repeat analysis carried out after more material has been removed from the sample base (by turning, milling) leads to larger systematic deviations in the mushroom sample than in the cylindrical sample. If material is removed from the samples, the composition of the remaining portion of sample no longer corresponds to the spoon sample (molten metal), which should be borne in mind when carrying out checks by wet chemistry.

    Direct sampling from melts can also be carried out using submerged moulds which are dipped into the melt. The inner space is covered with wood or some other material so that slag cannot run in when it is penetrated. After a few s the mould is so hot that the excess pressure forces the wooden cover off and metal flows in. The sample space contains a deoxidising agent. With this sampling technique, oxidation is much less than when pouring from a spoon through air into the mould. Scrap rates with submerged samples are 3 times higher(about 10%)than with samples poured by spoon into a mould.

    Direct sampling is also carried out using submergible probes/114/.This type of sample is sometimes called a "lollipop”, because of its shape. Steelworks are trying to reduce sampling and preparation times because of expensive furnace time. It is difficult to deoxidise unkilled steel in probes. X-ray examinations show gas bubbles sometimes larger than the metal volume in many samples.

     After 3 s it is full. The rapidly solidifying coin sample is removed by breaking up the ceramic front part. There are similar versions for sampling from melting units, ladles and moulds.

    The times required for sampling, transport and preparation are often many times longer than the analysis time at the spectrometer. It is possible to shorten the overall time by appropriate organisation and the use of optimum working aids in this area. At many melting plants today analysis is carried out on site /229/, and further progress is being made here with automation.

telephone:+86-15106177808
Tel:+86-0510-85598302
email:lm@chxyq.com

Address: 19th Liangtong Road, Mashan Town, Binhu District, Wuxi City, Jiangsu Province, China

Copyright ? 2015 All Rights Reserved

精品国产伦一区二区三区免费 _日韩欧美一区二区三区在线_欧美精品vⅰdeose4hd_91精品免费在线_欧美日韩国产一二三_色八戒一区二区三区_欧美日韩一级二级_欧美videos大乳护士334_欧美一区二区在线免费观看_{关键词10
欧美午夜电影网| 97精品视频在线观看自产线路二| 日韩美一区二区三区| 亚洲色图欧美偷拍| 5月丁香婷婷综合| 亚洲成人免费看| 亚洲第一久久影院| 福利一区福利二区微拍刺激| 在线播放国产精品二区一二区四区| 日韩欧美中文第一页| 国产精品国产三级国产aⅴ原创| 欧美色老头old∨ideo| 亚洲一区二区三区中文字幕在线| 精品人伦一区二区色婷婷| 美美哒免费高清在线观看视频一区二区| 欧美特级限制片免费在线观看| 国产乱对白刺激视频不卡| 精品免费一区二区三区| 在线观看亚洲a| 五月开心婷婷久久| 欧美少妇一区二区| 成人av集中营| 日韩毛片高清在线播放| 精品国产a毛片| 国产精品一区二区在线观看网站| 日韩欧美色综合网站| 精品久久久久久久久久国产| 综合在线观看色| 日本久久一区二区| 国产69精品久久99不卡| 国产精品美女久久久久久久| 精品三级在线观看| 成人理论电影网| 亚洲人成精品久久久久久| 色婷婷综合久久久中文字幕| 成人一区二区三区在线观看| 国产精品视频线看| 色综合色狠狠综合色| 波多野洁衣一区| 亚洲一二三四在线观看| 欧美日韩国产影片| 欧美在线不卡视频| 日本不卡视频在线| 欧美高清在线视频| 色婷婷亚洲精品| 欧美色videos| 蜜桃视频在线观看一区二区| 精品美女在线播放| 成人18视频在线播放| 亚洲综合免费观看高清完整版 | 精品国产91久久久久久久妲己 | 蜜臀国产一区二区三区在线播放 | 蜜桃av噜噜一区| 国产精品污www在线观看| 在线观看日韩高清av| 色综合久久久久| 韩国av一区二区三区四区| 在线视频国内一区二区| a4yy欧美一区二区三区| 午夜av一区二区三区| 久久久久久久网| 色琪琪一区二区三区亚洲区| 欧美性生活大片免费观看网址| 奇米一区二区三区| 欧美国产日本视频| 欧美日韩1区2区| 成人久久18免费网站麻豆| 亚洲一区二区高清| 久久久久久电影| 欧美久久一二区| 欧美一二三区在线| 欧美日韩中文字幕在线| 精品综合免费视频观看| 亚洲精品福利视频网站| 精品国产91乱码一区二区三区| 精品国产乱码久久| 欧美日韩国产片| 91亚洲永久精品| 国产酒店精品激情| 午夜精品久久久久久| 日韩久久一区二区| 久久婷婷成人综合色| 欧美乱妇23p| 精品国产乱码久久久久久闺蜜| 欧洲一区二区三区免费视频| 成人性视频网站| 麻豆精品视频在线观看| 亚洲国产精品综合小说图片区| 欧美极品xxx| 精品粉嫩aⅴ一区二区三区四区| 精品视频在线免费| 一本久道中文字幕精品亚洲嫩| 欧美日韩精品一区二区三区四区 | 欧美午夜精品免费| 91丨porny丨在线| 成人v精品蜜桃久久一区| 韩国视频一区二区| 日韩精品一级二级| 亚洲风情在线资源站| 亚洲欧美日韩国产成人精品影院| 欧美国产精品v| 久久精品网站免费观看| 精品国产乱码久久| 欧美不卡在线视频| 日韩一区二区视频在线观看| 欧美日韩国产片| 欧美日韩高清一区二区三区| 在线观看中文字幕不卡| 色久优优欧美色久优优| 精品国产sm最大网站免费看| 精品三级av在线| 精品久久久久av影院 | 91视频xxxx| 精品av在线播放| 欧美日韩免费观看中文| 91老师片黄在线观看| 色综合天天综合色综合av| 日韩av中文字幕一区二区 | 一区二区三区在线视频观看58 | 另类小说视频一区二区| 另类成人小视频在线| 久久99深爱久久99精品| 国产在线精品免费av| 国产精品一区二区久久精品爱涩| 国产精品18久久久久久久久| 国产成人自拍在线| 99久久精品情趣| 91久久奴性调教| 精品日韩欧美在线| 99re热视频精品| 不卡的看片网站| 国产福利91精品一区二区三区| 免费久久精品视频| 午夜一区二区三区视频| 一区二区国产盗摄色噜噜| 国产精品每日更新在线播放网址| 精品久久五月天| 日韩免费一区二区| 欧美日韩久久一区| 欧美午夜视频网站| 在线免费观看视频一区| 精品三级在线观看| 日韩一区二区免费在线电影| 天涯成人国产亚洲精品一区av| 亚洲一区日韩精品中文字幕| 日韩不卡一二三区| 国产寡妇亲子伦一区二区| 精品久久久久久久久久久久| xvideos.蜜桃一区二区| 亚洲欧美福利一区二区| 日本伊人午夜精品| 成人av免费在线| 欧美日韩一区高清| 在线视频欧美精品| 久久久噜噜噜久噜久久综合| 亚洲色图在线看| 伦理电影国产精品| 动漫精品一区二区| 欧美一区二区啪啪| 欧美一级夜夜爽| 成人欧美一区二区三区视频网页 | 亚洲尤物在线视频观看| 精品一区二区三区在线观看 | 欧美日韩国产大片| 欧美激情一区二区三区四区| 午夜伦理一区二区| 国产98色在线|日韩| 欧美日韩一区中文字幕| 欧美日韩综合在线免费观看| 国产欧美综合色| 午夜精品在线视频一区| 丁香啪啪综合成人亚洲小说| 欧美日韩国产系列| 欧美一个色资源| 一区二区三区国产精华| 国产不卡视频在线观看| 欧美日韩在线亚洲一区蜜芽| 666欧美在线视频| 亚洲欧洲日产国产综合网| 国模一区二区三区白浆| 在线免费亚洲电影| 91超碰这里只有精品国产| 亚洲欧洲制服丝袜| 成人激情小说乱人伦| 精品乱码亚洲一区二区不卡| 国产亚洲精品精华液| 美女视频一区二区三区| 欧美午夜电影在线播放| 3d动漫精品啪啪1区2区免费 | 国产精品灌醉下药二区| 国产乱淫av一区二区三区| 欧美日韩精品三区| 久久午夜老司机| 老汉av免费一区二区三区| 精品视频在线看| 精品久久人人做人人爱| 日韩va欧美va亚洲va久久| 日本成人超碰在线观看| 精品视频在线免费看| 精品国产一区二区三区四区四|